logo_footer
...
1.713916MnCrS5

 

 

1.7139 is a case hardening steel for steam boilers and turbines, shafts for higher temperature ranges

 

Composition:

 

%C%Si%Mn%P%SCrMoNiother
0,14-0,190,401,00-1,300,0350,02-0,0350,80-1,10

 

Hot working:

Forging temperature range: 1200-850℃
 
Note: Heat to 1200 ℃. Do not forge below 850.
 
Heat treatment:

Soft annealingHeat treatment to obtain a certain structureHeat treatment to obtain a certain tensile strengthCarburizeCore hardeningSurface hardeningTemper
650-700850-950900-1000900-950850-880810-840170-210

 

Main application:

Gear and link components, bevels, plate- and cog wheels
 
Shape of product:

Round, flat, step shape, ring, disc, shaft, other shape depend on customer needs